Cemented carbide is a significant type of cemented carbide, widely used in manufacturing cutting tools, wear-resistant parts, high-temperature alloy components, and other important applications. Factors such as extrusion forming processes, forming agents, sintering atmosphere, and magnetic properties all impact the performance and quality of WC+Co alloy. Studying the effects and mechanisms of these factors is crucial for optimizing the manufacturing process and enhancing the performance of cemented carbide. This article will explore the influence of sintering atmosphere and particle size on the quality of the extrusion forming process, providing theoretical and practical guidance for further understanding the manufacturing process and performance optimization of cemented carbide.

cemented carbide

Experimental Materials and Methods

Tungsten carbide (WC) powders were used as the raw material. Four different particle sizes of WC powder were selected: 4.0 μm, 2.2 μm, 1.1 μm, and 0.5 μm, which were labeled as WC1, WC2, WC3, and WC4, respectively. Metal cobalt (Co) powder was used as the binder phase, and paraffin was used as the forming agent. Four different WC-Co mixtures with varying particle sizes were prepared.

The mixtures were processed into green bodies with specific shapes and densities using extrusion forming equipment. The pressed green bodies were then placed in a sintering furnace and subjected to high-temperature sintering at 1400°C for 30 minutes, followed by cooling, to form cemented carbide bars.

The magnetic properties of the cemented carbide bars were tested using a magnetic performance tester, measuring parameters such as coercive force (Hc) and saturation magnetization (Bs), and the results were analyzed.

 

Experimental Results and Analysis

Table 1 presents the effects of different WC particle sizes on the coercive force (Hc) and saturation magnetization (Bs) of cemented carbide bars.
Table 1 presents the effects of different WC particle sizes on the coercive force (Hc) and saturation magnetization (Bs) of cemented carbide bars.

Effect of Particle Size on Coercive Force

As shown in Table 1, the coercive force of cemented carbide bars increases with decreasing WC particle size, while the saturation magnetization also increases. This indicates that cemented carbide bars made with fine and ultrafine WC particles exhibit poorer magnetic properties. Among the samples, the ultrafine WC (WC4) shows the highest coercive force of 4450 A/m, followed by medium-sized WC (WC3) with a coercive force of 3300 A/m. Coarse WC (WC2) and very coarse WC (WC1) have lower coercive forces, at 2350 A/m and 1200 A/m, respectively. The increase in coercive force with decreasing WC particle size is primarily due to the increase in internal defects and dislocations within smaller particles. These defects and dislocations create resistance to domain wall movement, making the magnetization process more difficult and requiring a larger external magnetic field to achieve saturation, thereby increasing the coercive force.

 

Effect of Particle Size on Material Magnetic Performance Stability

For fine and ultrafine WC particles, the larger grain boundary area facilitates grain boundary diffusion and reactions, which reduces the material’s magnetic properties. As the WC particle size decreases, the magnetic saturation of cemented carbide bars gradually increases. Specifically: coarse WC (WC1) exhibits the lowest magnetic saturation at only 1.25 T; medium-sized WC (WC2) has a magnetic saturation of 1.15 T; fine WC (WC3) and ultrafine WC (WC4) show higher magnetic saturations at 1.05 T and 0.93 T, respectively. This is likely because fine and ultrafine WC particles have higher chemical reactivity, promoting the diffusion and bonding of the Co binder, thereby improving the stability of the material’s magnetic performance.

Magnetic saturation is an indicator of the remaining proportion of magnetizable material and is closely related to magnetic properties such as coercive force and remanence. The impact of WC particle size on magnetic saturation can be attributed to the degree of solubility of the binder phase in the cemented carbide bars. Coarse and medium-sized WC particles, having larger specific surface areas, have more contact with the Co binder, which enhances the solubility of Co in the cemented carbide bars. This effectively improves the material’s magnetic performance stability, resulting in higher coercive force and better magnetic stability. Conversely, fine and ultrafine WC particles, with smaller specific surface areas, reduce the effectiveness of the Co binder, potentially affecting the material’s hardness and magnetic properties. Thus, selecting the appropriate particle size during the preparation of cemented carbide bars is crucial for achieving the best overall performance based on specific application needs.

 

Impact of Gamma Phase on Material Performance

For cemented carbide materials, the proportion of the gamma phase directly affects the material’s hardness and magnetic properties. Variations in carbon and oxygen content also influence the gamma phase proportion and must be considered during material preparation. Generally, higher carbon content leads to an increase in the gamma phase proportion, thereby enhancing the material’s hardness and magnetic performance. Therefore, different WC particle sizes may have varying carbon and oxygen contents, which also affects the gamma phase proportion and the overall performance of the material.

 

Discussion on Sintering Atmosphere

In the sintering process of cemented carbides, the choice and control of the atmosphere have a decisive impact on the final microstructure and magnetic properties of the material. The atmosphere not only affects the chemical reactions during sintering but also directly relates to the microstructure and final performance of the cemented carbide. The types of sintering atmospheres are as follows:

Oxidizing Atmosphere:? air.

Reducing Atmosphere: Contains components such as H? or CO: hydrogen atmosphere for cemented carbide sintering.

Inert or Neutral Atmosphere: Argon, helium, vacuum.

Carburizing Atmosphere: Contains high components that cause carburization of the sintered body, such as CO, methane, and hydrocarbon gases.

Nitrogen-Based Atmosphere: High nitrogen content sintering atmosphere: 10% H? in N?.

We mainly selected vacuum, argon, and hydrogen atmospheres for discussion. The variations in coercive force and magnetic saturation of cemented carbides sintered in argon, vacuum, and hydrogen atmospheres differ depending on the atmosphere, as shown in Table 2.

Table 2: Effects of Different Sintering Atmospheres on Magnetic Properties of Cemented Carbide Bars
Table 2: Effects of Different Sintering Atmospheres on Magnetic Properties of Cemented Carbide Bars

From Table 2, it can be observed that under vacuum and argon atmospheres, the coercive force (Hc) of cemented carbide bar is higher compared to that in a hydrogen atmosphere. Conversely, the saturation magnetization (Bs) is lowest in a hydrogen atmosphere compared to vacuum and argon atmospheres.

Under vacuum and argon atmospheres, the effective control of oxygen partial pressure and the exclusion of volatile elements result in fewer pores and inclusions, clearer grain boundaries, and better grain growth, thereby enhancing the magnetic properties of the material. In contrast, in a hydrogen atmosphere, the reducing nature of hydrogen may reduce some elements in the cemented carbide, leading to the presence of uncertain phase components, poor grain growth, and subsequently affecting the material’s magnetic properties.

For coercive force (Hc), it is largely dependent on the material’s microstructure and magnetic anisotropy. Under vacuum and argon atmospheres, effective control of oxygen partial pressure and exclusion of volatile elements reduce magnetic anisotropy in the cemented carbide, which improves coercive force. However, in a hydrogen atmosphere, hydrogen’s reducing effect can lead to the reduction of some elements in the cemented carbide, resulting in grain defects and inclusions that directly affect magnetic anisotropy and reduce coercive force.

Regarding saturation magnetization (Bs), the relative magnetic saturation value in cemented carbide is influenced by factors affecting carbon content in the alloy. In vacuum or argon atmospheres, effective control of oxygen content reduces carbon loss. Although the pressed green body contains oxygen, which can be reduced by free carbon and carbon in WC (MeO + C = Me + CO), the oxygen content in these atmospheres is relatively low. In a hydrogen atmosphere, decarburization reactions (WC + 2H? → CH? + C) begin at around 100°C. Throughout the preparation process, the material is exposed to a decarburizing atmosphere, leading to a lower relative magnetic saturation value.

How Do Sintering Atmosphere and Particle Size Affect the Extrusion Forming Quality of Cemented Carbide Bars? 2

結(jié)論

This experiment investigated the effects of different particle sizes and sintering atmospheres on the magnetic properties of cemented carbide bars. By comparing the magnetic properties of cemented carbide under different WC particle sizes (coarse, medium, fine, and ultrafine) and sintering atmospheres (vacuum, argon, and hydrogen), it was found that both particle size and atmosphere have a significant impact on the magnetic performance of the material.

From the perspective of particle size, as the WC particle size decreases, the coercive force of the cemented carbide bars increases, while magnetic saturation also increases. This indicates that particle size has a substantial effect on the magnetic properties of cemented carbide. Fine and ultrafine WC particles, due to their higher chemical reactivity and good sintering performance, can promote the diffusion and bonding of the Co binder, thus enhancing the stability of the material’s magnetic performance. However, smaller particle sizes may lead to increased porosity and inclusions, affecting the material’s hardness and magnetic performance. Therefore, the choice of particle size should be tailored to the specific application needs when preparing cemented carbide.

Regarding the atmosphere, cemented carbide bars sintered under vacuum and argon atmospheres exhibited higher coercive force and better magnetic stability. This is because these atmospheres effectively control the oxygen content and volatile elements, reducing porosity and inclusions, and promoting clearer grain boundaries and grain growth. In contrast, cemented carbide bars sintered in a hydrogen atmosphere showed significantly lower magnetic saturation. This is likely due to the decarburizing effect of hydrogen. Therefore, selecting the appropriate sintering atmosphere is crucial for obtaining cemented carbide bars with excellent magnetic properties. Further improvements in cemented carbide performance can be achieved by optimizing sintering process parameters and adding suppressants.

9 月 4, 2024

Meilleur matériaux TOP

發(fā)表評(píng)論

電子郵件地址不會(huì)被公開(kāi)。 必填項(xiàng)已用*標(biāo)注

日本高清一区二区三区在线观看| 国产精品一区二区三区涩涩av| 国产精品久久一区二区三区动| 男人添女人下面免費视頻| 另类 专区 综合 中文| 成人av大全免费一区二区三区| 视频在线观看一区@99| 女人扒开腿让我舔十八禁| 男人把鸡巴插入女人| 日韩亚洲AV无码一区二区不卡| 精品一区二区久久久久无码| 国产伦精品一区二区三区福利| 黄色亚洲一级大片| 亚洲中文字幕在线无码一区二区| 中日美女毛5片一区二区三区| 黑丝美女被操哭边操边尿| 女女同性女同1区二区三| 美女大鸡操很多水在线看| 操逼啊 啊 啊黄色视频| 日韩欧美一二三区| 日本精品久久不卡一区二区| 国产 日韩 亚洲 一区| 日韩高清毛片在线观看| 久久综合色鬼综合色| 插逼爽歪歪视频免费| 亚洲精品成a人在线观看| 黄色高清带三级1集2集| 东京热无码AV一区二区三区| 精品一区二区久久久久无码| 日韩精品高清在线| 亚洲国产综合精品 在线 一区| 国产精品高潮久久久久a| 亚洲一区二区三区四区国产| 日韩欧美一区二三区风间由美| 鸡巴操骚逼视频播放| 99久久久国产精品k影| 大鸡巴射在穴穴里的视频| 欧美人与兽大屌肛交爆菊| 欧美亚洲综合久久夜夜嗨| 大鸡巴狂插嫩逼视频| 国产精品日韩精品欧美精品|