Quenching crack is a common quenching defect, which is caused by many factors. Because the defects of heat treatment begin with product design, the work of preventing cracks should start with product design. It is necessary to select materials correctly and design structures rationally, put forward appropriate technical requirements for heat treatment, properly arrange technological route, select reasonable heating temperature, holding time, heating medium, cooling medium, cooling method and operation mode, etc.

Material aspect

1. Carbon is an important factor affecting quenching tendency. With the increase of carbon content, MS point decreases and quenching tendency increases. Therefore, under the condition of satisfying the basic properties such as hardness and strength, the lower carbon content should be chosen as far as possible to ensure that it is not easy to quench.

2. The influence of alloying elements on quenching tendency is mainly reflected in the influence on hardenability, MS point, grain size growth tendency and decarbonization. The alloying elements affect the tendency of quenching by influencing the hardenability. Generally speaking, the hardenability increases and the cracking ability increases, but when the hardenability increases, the quenching medium with weak cooling ability can be used to reduce the quenching deformation to prevent the deformation and cracking of complex parts. Therefore, for complex parts, in order to avoid quenching cracks, it is a better scheme to select steel with good hardenability and use quenching medium with weak cooling capacity.

Generally speaking, the lower the MS, the greater the tendency of quenching. When the MS point is high, the martensite formed by transformation may be self-tempered immediately, thus eliminating part of the transformation stress and avoiding the occurrence of quenching. Therefore, when the carbon content is determined, a small amount of alloying elements should be selected, or steel grades containing elements which have little influence on MS point should be selected.

3. Superheat sensitivity should be considered when selecting steel. Overheat sensitive steel is prone to cracks, so attention should be paid to the selection of materials.

Structural Design of Parts

1. Uniform cross-section size.

Cracks occur in parts with sharply varying cross-section size due to internal stress during heat treatment. Therefore, the sudden change of section size should be avoided as far as possible in design. The wall thickness should be uniform. If necessary, openings may be made in thick-walled parts which have no direct relationship with the use. Holes should be made through as much as possible. For parts with different thicknesses, separate design can be carried out, and then assembled after heat treatment.

2. Round corner transition.

When the parts have edges, sharp corners, grooves and transverse holes, these parts are prone to stress concentration, leading to parts quenching. For this reason, parts should be designed as far as possible to avoid stress concentration, and processed into rounded corners at sharp corners and steps.

3. The difference of cooling rate caused by shape factor.

The cooling speed of parts during quenching varies with the shape of parts. Even in different parts of the same part, the cooling rate varies due to various factors. Therefore, excessive cooling differences should be avoided to prevent quenching cracks.

Technical Conditions for Heat Treatment

1. Use local quenching or surface hardening as far as possible.

2. To adjust the local hardness of quenched parts reasonably according to the requirement of service conditions of parts. When the local quenching hardness requirement is low, try not to force the overall hardness to be the same.

3. Pay attention to the quality effect of steel.

4. Avoid tempering in the first kind of tempering brittle zone.

5. Reasonable arrangement of process route and process parameters: Once the material, structure and technical conditions of steel parts are determined, the heat treatment technicians will carry out process analysis to determine a reasonable process route, that is, to correctly arrange the position of preparation heat treatment, cold processing and hot processing and determine the heating parameters.

Quenching Crack

At 1,500X, the crack is serrated, the crack at the beginning is wide, and the fracture lines at the end are small to none.

 fracture lines

2. Microscopic analysis: abnormal metallurgical inclusions, crack morphology is zigzag extension; after corrosion with 4% nitric acid alcohol, there is no decarbonization phenomenon, the microscopic morphology is shown in the following figure:

decarbonization phenomenon

1 # Sample

No abnormal metallurgical inclusions and decarbonization were found in the cracks. The cracks extend in zigzag shape and have the typical characteristics of quenching cracks.

quenching crack

2 # Samples

Analytical conclusions:

1. The composition of the sample meets the requirements of the standard and corresponds to the original furnace number.

2. According to the microscopic analysis, no abnormal metallurgical inclusions and decarbonization were found at the cracks of the samples. The cracks extend in zigzag shape and have the typical characteristics of quenching cracks.

Forging cracks

1. Cracks caused by typical material causes, with oxide edges.

  • Microscopic observation
Microscopic observation
  • Microscopic observation
 decarburization depth

The surface white bright layer should be secondary quenched layer, and the deep black layer under secondary quenched layer should be high temperature tempered layer.

It is concluded that cracks with decarburization need to be distinguished from raw material cracks. Generally, the forging cracks whose decarburization depth is greater than or equal to surface decarburization depth are raw material cracks, and the forging cracks whose decarburization depth is less than surface decarburization depth.

伊人久久综合无码成人网| 九九在线视频热线视频精选| 91video国产一区| 日韩欧美一区二三区风间由美| 无码视频在线观看| 大香蕉中码手机在线视频| 久久久久九九九国产精品| 国产又粗又猛又色又免费| 天美传媒精品1区2区3区| 被下药强奷到舒服的视频| 99视频在线看免费视频| 亚洲国产成久久成人综合一区| 成人精品视频区一区二区三| 野外日逼视频免费看| 三上悠亚精品一区二区久久| 男女操逼视频嫩嫩| 在线观看国产日韩欧美一区二区| 精品久久久久久久人妻换| 瓯美在线免费视频笫一区第二区| 午夜十八禁福利亚洲一区二区| 日日爱黄色毛片视频| 久久免费国产视频| 亚洲一区二区三区大胆视频| 999精品免费视频| 欧美日韩综合在线一区| 欧美日韩久久久一区二区三区| 国产午夜爽爽爽男女免费动漫AV| 欧美巨屌虐无毛骚逼| 精品免费久久久久久久久| 亚洲国产精品一区亚洲国产| 淫荡扣逼骚逼视频| 日韩欧美一区二区三区在线视频| 色偷偷影音先锋男人av| 骚女人被大吊干视‘| 亚洲大尺度无码无码专线一区| 丁香婷婷色婷婷粗大| 国产品无码一区二区三区在线| 白色紧身裤无码系列在线| 黑人妖大鸡吧操逼| 欧美一区二区三区四区五区精品| 精品免费在线观看等|