Tungsten carbide roll rings (WC rolls) are high-performance rolling mill components made from tungsten carbide (WC) particles bonded with cobalt (Co) or nickel (Ni) through powder metallurgy. They are widely used in high-speed wire rod mills, bar mills, and section mills due to their exceptional wear resistance, thermal stability, and strength.

They can be usefully used for finishing stands of high-speed wire rod mills (up to 120 m/s),precision rolando of rebars, alloy steels, and non-ferrous metals, and high-reduction passes where wear resistance is critical

Practical condition

Located in Guangdong Province, A metal production company commissioned its high-speed wire rod mill (with an annual capacity of 1.2 million tons of φ5.5~φ16mm wire rods) in December 2010 to enhance production efficiency and meet market demands.

The mill primarily consists of five key components: roughing mill, intermediate mill, pre-finishing mill, and finishing mill. The roughing mill features a single-line configuration with 5 stands (φ550×5) arranged in horizontal-horizontal-vertical-horizontal-vertical (HHVHV) pattern. The intermediate mill comprises 8 stands (φ550×2+φ450×4+φ350×2) with all-horizontal rolls. The pre-finishing mill has 8 stands (dual-line, 4 stands per line) configured as cantilever-type two-high mills (φ285×4×2) with alternating horizontal/vertical arrangement. The finishing mill contains 20 stands (dual-line, 10 stands per line) of cantilever-type two-high mills (gang-driven, φ228×5+φ170×5) in 45° top-cross configuration.

Due to humid climatic conditions, the mill encountered roll ring explosions caused by moisture-induced rusting of roll rings and taper sleeves. A technical task force was established to identify root causes and implement corrective measures to ensure stable production.

Practical Investigation and Solutions for Roll Ring Fractures in High-Speed Wire Rod Production 2

Production Process Overview

The manufacturing process flows as follows:

1.After single-pass rolling in the roughing mill, the billet undergoes head/tail cropping at #1 flying shear (with emergency scrap chopping capability), then diverges into dual lines via a distributor for intermediate rolling under micro-tension control.

2.Following intermediate rolando, the stock passes through #2 flying shear for cropping before entering pre-finishing mill, where pneumatic vertical loopers enable twist-free, tensionless rolling for precise dimensional control.

3.Pre-finished stock undergoes water cooling and #3 flying shear cropping before entering finishing mill. Emergency shutoff shears activate to prevent further stock entry during malfunctions.

4.The 45° top-cross finishing mill employs gang-driven tungsten carbide roll rings for twist-free micro-tension rolling, achieving final dimensions at speeds up to 95m/s for φ5.5~7mm products.

carbide roll rings

Root Cause Analysis of Roll Ring Failures

The cost-optimized tungsten carbide roll rings exhibited these failure mechanisms:

Ambient humidity caused rust corrosion at roll ring/taper sleeve interfaces

Thermal fatigue from cyclic temperature variations (Fig.1) accelerated crack propagation

Insufficient cooling exacerbated thermal stresses (increased ΔT)

Improper assembly caused taper sleeve seizure

Brittle material properties increased handling damage risks

 

Technical Improvements & Process Controls

Material Selection Optimization

The YGR-series roll rings were selected for their Ni/Cr-enhanced properties:

1.Superior oxidation resistance (700-1000℃)

2.Improved acid corrosion resistance (pH≤7.2)

3.Enhanced thermal crack resistance

4.Optimal hardness-toughness balance across mill stands

 

Cooling System Enhancements

Implemented strict water management protocols:

1.Flow rates: 18-25m3/h per stand (slot-width dependent)

2.Pressure maintenance: 3-7bar at nozzles

3.Monthly water quality testing for particulate control

Dedicated pipe alignment inspections during maintenance

 

Optimum Rolling Tonnage

Established safe grinding thresholds at 0.2-0.4mm crack depth:

Stands 1-4: 1,800-2,500 tons

Stands 5-8: 1,500-2,000 tons

Stands 9-10: 600-1,000 tons

 

Precision Assembly Standards

Mandatory surface cleaning before assembly

Prohibited impact mounting methods

Individual roll storage in partitioned containers

Strict taper sleeve inspection/rejection criteria

 

Conclus?o

The comprehensive improvement program addressing material selection, cooling optimization, production control, and precision maintenance successfully resolved roll ring failures, achieving sustained operational stability. This methodology provides valuable reference for similar applications.

Key Recommendations

1.Select roll ring grades considering environmental factors

2.Maintain rigorous cooling water quality standards

3.Adhere to prescribed rolling tonnage limits

4.Implement precision handling and maintenance protocols

Deixe uma resposta

O seu endere?o de e-mail n?o será publicado. Campos obrigatórios s?o marcados com *

狠狠色伊人亚洲综合成人| 美女穿黑丝被大鸡巴猛操| 精品精品国产一区二区性色av| 女人被躁到高潮嗷嗷叫小| 久久精品国产亚洲高清| 久久精品欧美精品免费观看| 国产精品熟女一区二区三区久久夜| 久久久五月性色视频| 美女穿黑丝被大鸡巴猛操| 免费人成再在线观看| 欧美综合区自拍亚洲综合| 日韩av一区二区高清不卡| 国产成人精品免费视频全| 日本高清一区二区三区水蜜桃| 久久精品一区二区三区免费看| 中文字幕乱码人妻一区二区三区| 国产乱子伦视频一区二区三区| 爆乳喷奶水无码正在播放| 天美传媒精品1区2区3区| 黑人妖大鸡吧操逼| 大鸡吧干小逼逼视频大全| 啊好爽好多水深插射视频| 欧美另类在线观看| 嗯嗯好硬好大啊老公| 黑大吊肏小騷逼噴水| 啊啊啊男女激情插插视频| 日本不卡高清视频在线播放| 国产精品欧美久久久久久| 这里只有久久精品| 中国老女人 操逼 视频| 91孕妇精品一区二区三区| 日韩美女一区二区三区香蕉视频| 美女爽的嗷嗷叫免费| 插女生那个的视频| 少妇无套带白浆嗯呢啊污| 白丝袜子宫啊啊啊不要了| 久久一区二区三区精华液介绍| 男人和女人干污污| 久久久国产精品2020| 老熟妇高潮一区二区高清视频| 裸体美女被操的啊啊直叫|