欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 1

Spherical Cast Tungsten Carbide Powder is a novel type of highly wear-resistant ceramic particle material. Compared to traditional tungsten carbide, spherical cast tungsten carbide possesses two significant advantages. Firstly, it has a regular spherical appearance with good powder flowability and wetting properties. When used as an additive particle, it exhibits excellent compatibility with the surrounding structure, reducing stress concentration. Secondly, the internal structure of the tungsten carbide particles is dense, exhibiting good toughness, fine grain size, high hardness, and excellent wear resistance as a coating. It is less prone to fracture under load.

Due to its outstanding performance, spherical cast tungsten carbide powder is gradually replacing traditional tungsten carbide powder in surface protection applications for mining machinery, petroleum machinery, construction industry, and foundries. It significantly enhances the wear resistance, corrosion resistance, and oxidation resistance of components, thereby extending their service life.

The chemical composition, microscopic morphology, microstructure, microhardness, and other powder properties of spherical cast tungsten carbide powder prepared by different methods will be investigated below.

The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 2

1.Chemical composition of sample carbide powder

The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 3

The table above shows the chemical composition of spherical cast tungsten carbide powder samples prepared by different methods. It can be observed that the main components of spherical cast tungsten carbide powder are tungsten (W) and carbon (C), with trace amounts of iron (Fe), vanadium (V), chromium (Cr), and niobium (Nb). The ideal composition of spherical cast tungsten carbide should consist of eutectic WC and W2C phases, with a eutectic temperature of 2525 ℃ and a carbon content of 3.840% (mass fraction) at the eutectic point. From the data in the table, it can be seen that the spherical cast tungsten carbide powder prepared by the plasma rotating electrode atomization method has the smallest deviation from the theoretical carbon content and the lowest free carbon content. On the other hand, the powder obtained from the induction melting and atomization method shows the largest deviation from the theoretical carbon content, with a difference of 0.170% (mass fraction). This is likely due to the use of graphite tube heating in the induction melting process, which can increase the carbon content. Therefore, compared to other methods, the plasma rotating electrode atomization method can more accurately control the carbon content of spherical cast tungsten carbide powder, preventing over-eutectic and sub-eutectic reactions caused by carburization and decarburization, and achieving a near-perfect eutectic microstructure. This is crucial for improving the microstructure and properties of spherical cast tungsten carbide.

2.Microscopic morphology

fig1.The microstructure of spherical cast tungsten carbide powder samples
fig1.The microstructure of spherical cast tungsten carbide powder samples

The figure above shows the microstructure of spherical cast tungsten carbide powder prepared by different methods. It can be observed that the spherical cast tungsten carbide powder obtained from all three methods exhibits a regular and smooth near-spherical shape.

The cross-sectional images of spherical cast tungsten carbide powder
fig.2 The cross-sectional images of spherical cast tungsten carbide powder

The figure above shows cross-sectional photographs of spherical cast tungsten carbide powder prepared by different methods. From (a) and (b), it can be observed that the particles of spherical tungsten carbide powder prepared by plasma rotating electrode atomization method have a dense internal structure with almost no defects. However, from (c) and (d), it can be seen that spherical tungsten carbide powder prepared by plasma melting and atomization as well as induction melting and atomization methods have some noticeable pores or hollow particles within their internal structure. The main reason for this is that the crushed tungsten carbide powder used as raw material in the above-mentioned methods may contain residual pores from the casting process. During the short-duration plasma or induction heating process, it becomes challenging for the internal part of the crushed tungsten carbide powder to fully melt, resulting in the presence of some pores within the particles.

3.Microstructure

the microscopic structure of spherical cast tungsten carbide powder samples
fig3. the microscopic structure of spherical cast tungsten carbide powder samples

The figure above displays microscopic images of the microstructure of spherical cast tungsten carbide powder particles prepared by different methods after corrosion. It can be observed that the internal structure of the particles in all three methods primarily consists of a typical fine needle-like eutectic structure of WC and W2C phases. Compared to plasma melting and atomization and induction melting and atomization methods, the eutectic microstructure of spherical cast tungsten carbide powder obtained by plasma rotating electrode atomization method appears to be finer and denser. This is because, in contrast to plasma melting and atomization and induction melting and atomization methods, plasma rotating electrode atomization method fully melts the tungsten carbide raw material rod and rapidly solidifies it under the centrifugal force. The higher undercooling during the crystallization of the molten tungsten carbide results in more rapid nucleation and a greater number of crystal nuclei formation, leading to a finer eutectic microstructure.

4.Microhardness

The table below shows the average microhardness of spherical cast tungsten carbide powder prepared by different methods. It can be observed that the microhardness of the spherical cast tungsten carbide powder obtained from all three methods is above 2800 HV0.1. Among them, the powder produced by the plasma rotating electrode atomization method exhibits the highest microhardness, reaching 3045 HV0.1. This is mainly due to the finer and denser eutectic microstructure within the spherical cast tungsten carbide powder obtained by the plasma rotating electrode atomization method.

The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 4

5.Other physical properties

The table below presents the flowability and tap density values of spherical cast tungsten carbide powder prepared by different methods. It can be observed that the powder obtained from the plasma rotating electrode atomization method has the poorest flowability and the lowest tap density. On the other hand, the powder obtained from the induction melting and atomization method exhibits the best flowability and the highest tap density.

The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 5

Conclusione

(1) The spherical cast tungsten carbide powder prepared by the plasma rotating electrode atomization method exhibits the smallest deviation from the theoretical carbon content and eutectic carbon content, with the lowest free carbon content and relatively low impurity content.

(2) The internal structure of the spherical tungsten carbide powder particles obtained by the plasma rotating electrode atomization method is dense, with almost no defects. The eutectic microstructure is finer and denser. On the other hand, the particles obtained by plasma melting and atomization as well as induction melting and atomization methods show some noticeable pores or hollow particles within their internal structure.

(3) All three methods result in spherical cast tungsten carbide powder primarily consisting of WC and W2C phases.

(4) The microhardness of the spherical cast tungsten carbide powder obtained by all three methods is above 2800 HV0.1. Among them, the powder produced by the plasma rotating electrode atomization method exhibits the highest microhardness, reaching 3045 HV0.1. The powder obtained by the induction melting and atomization method shows good flowability and the highest tap density.

The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 6

The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 7

 

 

 

 

Luglio 16, 2023

Hello. I work in the aviation sector and we are metal strip drawing SS aviation grade metal and cannot seem to find a carbide that gives us the toughness and long wear properties that normal carbide would provide with regular tungsten carbide used in metal drawing of softer materials?Would you have a supplier list of companies that provide this new type of carbide? Regards

Agosto 3, 2023

Hello Dale,
Thank you for leaving a comment!
Could you please send us an inquiry to [email protected]?
Distinti saluti,

Lascia un commento

Il tuo indirizzo email non sarà pubblicato. I campi obbligatori sono contrassegnati *

男女边吃奶边做边爱视频| 亚洲二亚洲欧美一区vr| 久久久18禁一区二区网| 国产精品免费99久久久| 大鸡插骚货人人色| 看看美日韩操逼吧| 国产色哟哟精选在线播放| 一区二区三区中文字幕免费在线| 大阴茎交于大阴户黄片视频| 亚洲av 又黄又爽十大| 久久久精品欧美一区二区三免费| 骚女人被大吊干视‘| 色偷偷影音先锋男人av| 久久高清中文字幕第一页| 成人久久久久久蜜桃免费| 大肉棒插了按摩视频| 日逼动态视频免费看| 久久综合娱乐中文网| 欧美日韩一区精品一区精品| 娇嫩的被两根粗大的np| 色999日韩自偷自拍美女| 大鸡巴插入骚穴在线观看| 日韩 欧美 一区 二区三区| 中日美女毛5片一区二区三区| 日本亚洲免费不卡| 韩国精品视频一区二区在线观看| 国产 自拍 欧美 在线| 一级做a爱过程免费视频俩| 女生的鸡鸡色色软件| 男人操女人黄片黄色| 淫荡淫水逼操烂视频| 24日本精品视频免费| 99爱国产精品免费视频| 国产试看精品无码中| 欲色福利网免费在线播放| 大鸡巴操屁眼无码| 中文字幕在线观一区二区| 几巴怪物操逼视频| 日本一区二区三区高潮喷吹| 日韩素人精品亚洲热一区| 日本av在线一区二区|