Cemented carbide is a significant type of cemented carbide, widely used in manufacturing cutting tools, wear-resistant parts, high-temperature alloy components, and other important applications. Factors such as extrusion forming processes, forming agents, sintering atmosphere, and magnetic properties all impact the performance and quality of WC+Co alloy. Studying the effects and mechanisms of these factors is crucial for optimizing the manufacturing process and enhancing the performance of cemented carbide. This article will explore the influence of sintering atmosphere and particle size on the quality of the extrusion forming process, providing theoretical and practical guidance for further understanding the manufacturing process and performance optimization of cemented carbide.

cemented carbide

Experimental Materials and Methods

Tungsten carbide (WC) powders were used as the raw material. Four different particle sizes of WC powder were selected: 4.0 μm, 2.2 μm, 1.1 μm, and 0.5 μm, which were labeled as WC1, WC2, WC3, and WC4, respectively. Metal cobalt (Co) powder was used as the binder phase, and paraffin was used as the forming agent. Four different WC-Co mixtures with varying particle sizes were prepared.

The mixtures were processed into green bodies with specific shapes and densities using extrusion forming equipment. The pressed green bodies were then placed in a sintering furnace and subjected to high-temperature sintering at 1400°C for 30 minutes, followed by cooling, to form cemented carbide bars.

The magnetic properties of the cemented carbide bars were tested using a magnetic performance tester, measuring parameters such as coercive force (Hc) and saturation magnetization (Bs), and the results were analyzed.

 

Experimental Results and Analysis

Table 1 presents the effects of different WC particle sizes on the coercive force (Hc) and saturation magnetization (Bs) of cemented carbide bars.
Table 1 presents the effects of different WC particle sizes on the coercive force (Hc) and saturation magnetization (Bs) of cemented carbide bars.

Effect of Particle Size on Coercive Force

As shown in Table 1, the coercive force of cemented carbide bars increases with decreasing WC particle size, while the saturation magnetization also increases. This indicates that cemented carbide bars made with fine and ultrafine WC particles exhibit poorer magnetic properties. Among the samples, the ultrafine WC (WC4) shows the highest coercive force of 4450 A/m, followed by medium-sized WC (WC3) with a coercive force of 3300 A/m. Coarse WC (WC2) and very coarse WC (WC1) have lower coercive forces, at 2350 A/m and 1200 A/m, respectively. The increase in coercive force with decreasing WC particle size is primarily due to the increase in internal defects and dislocations within smaller particles. These defects and dislocations create resistance to domain wall movement, making the magnetization process more difficult and requiring a larger external magnetic field to achieve saturation, thereby increasing the coercive force.

 

Effect of Particle Size on Material Magnetic Performance Stability

For fine and ultrafine WC particles, the larger grain boundary area facilitates grain boundary diffusion and reactions, which reduces the material’s magnetic properties. As the WC particle size decreases, the magnetic saturation of cemented carbide bars gradually increases. Specifically: coarse WC (WC1) exhibits the lowest magnetic saturation at only 1.25 T; medium-sized WC (WC2) has a magnetic saturation of 1.15 T; fine WC (WC3) and ultrafine WC (WC4) show higher magnetic saturations at 1.05 T and 0.93 T, respectively. This is likely because fine and ultrafine WC particles have higher chemical reactivity, promoting the diffusion and bonding of the Co binder, thereby improving the stability of the material’s magnetic performance.

Magnetic saturation is an indicator of the remaining proportion of magnetizable material and is closely related to magnetic properties such as coercive force and remanence. The impact of WC particle size on magnetic saturation can be attributed to the degree of solubility of the binder phase in the cemented carbide bars. Coarse and medium-sized WC particles, having larger specific surface areas, have more contact with the Co binder, which enhances the solubility of Co in the cemented carbide bars. This effectively improves the material’s magnetic performance stability, resulting in higher coercive force and better magnetic stability. Conversely, fine and ultrafine WC particles, with smaller specific surface areas, reduce the effectiveness of the Co binder, potentially affecting the material’s hardness and magnetic properties. Thus, selecting the appropriate particle size during the preparation of cemented carbide bars is crucial for achieving the best overall performance based on specific application needs.

 

Impact of Gamma Phase on Material Performance

For cemented carbide materials, the proportion of the gamma phase directly affects the material’s hardness and magnetic properties. Variations in carbon and oxygen content also influence the gamma phase proportion and must be considered during material preparation. Generally, higher carbon content leads to an increase in the gamma phase proportion, thereby enhancing the material’s hardness and magnetic performance. Therefore, different WC particle sizes may have varying carbon and oxygen contents, which also affects the gamma phase proportion and the overall performance of the material.

 

Discussion on Sintering Atmosphere

In the sintering process of cemented carbides, the choice and control of the atmosphere have a decisive impact on the final microstructure and magnetic properties of the material. The atmosphere not only affects the chemical reactions during sintering but also directly relates to the microstructure and final performance of the cemented carbide. The types of sintering atmospheres are as follows:

Oxidizing Atmosphere:? air.

Reducing Atmosphere: Contains components such as H? or CO: hydrogen atmosphere for cemented carbide sintering.

Inert or Neutral Atmosphere: Argon, helium, vacuum.

Carburizing Atmosphere: Contains high components that cause carburization of the sintered body, such as CO, methane, and hydrocarbon gases.

Nitrogen-Based Atmosphere: High nitrogen content sintering atmosphere: 10% H? in N?.

We mainly selected vacuum, argon, and hydrogen atmospheres for discussion. The variations in coercive force and magnetic saturation of cemented carbides sintered in argon, vacuum, and hydrogen atmospheres differ depending on the atmosphere, as shown in Table 2.

Table 2: Effects of Different Sintering Atmospheres on Magnetic Properties of Cemented Carbide Bars
Table 2: Effects of Different Sintering Atmospheres on Magnetic Properties of Cemented Carbide Bars

From Table 2, it can be observed that under vacuum and argon atmospheres, the coercive force (Hc) of cemented carbide bar is higher compared to that in a hydrogen atmosphere. Conversely, the saturation magnetization (Bs) is lowest in a hydrogen atmosphere compared to vacuum and argon atmospheres.

Under vacuum and argon atmospheres, the effective control of oxygen partial pressure and the exclusion of volatile elements result in fewer pores and inclusions, clearer grain boundaries, and better grain growth, thereby enhancing the magnetic properties of the material. In contrast, in a hydrogen atmosphere, the reducing nature of hydrogen may reduce some elements in the cemented carbide, leading to the presence of uncertain phase components, poor grain growth, and subsequently affecting the material’s magnetic properties.

For coercive force (Hc), it is largely dependent on the material’s microstructure and magnetic anisotropy. Under vacuum and argon atmospheres, effective control of oxygen partial pressure and exclusion of volatile elements reduce magnetic anisotropy in the cemented carbide, which improves coercive force. However, in a hydrogen atmosphere, hydrogen’s reducing effect can lead to the reduction of some elements in the cemented carbide, resulting in grain defects and inclusions that directly affect magnetic anisotropy and reduce coercive force.

Regarding saturation magnetization (Bs), the relative magnetic saturation value in cemented carbide is influenced by factors affecting carbon content in the alloy. In vacuum or argon atmospheres, effective control of oxygen content reduces carbon loss. Although the pressed green body contains oxygen, which can be reduced by free carbon and carbon in WC (MeO + C = Me + CO), the oxygen content in these atmospheres is relatively low. In a hydrogen atmosphere, decarburization reactions (WC + 2H? → CH? + C) begin at around 100°C. Throughout the preparation process, the material is exposed to a decarburizing atmosphere, leading to a lower relative magnetic saturation value.

How Do Sintering Atmosphere and Particle Size Affect the Extrusion Forming Quality of Cemented Carbide Bars? 2

Fazit

This experiment investigated the effects of different particle sizes and sintering atmospheres on the magnetic properties of cemented carbide bars. By comparing the magnetic properties of cemented carbide under different WC particle sizes (coarse, medium, fine, and ultrafine) and sintering atmospheres (vacuum, argon, and hydrogen), it was found that both particle size and atmosphere have a significant impact on the magnetic performance of the material.

From the perspective of particle size, as the WC particle size decreases, the coercive force of the cemented carbide bars increases, while magnetic saturation also increases. This indicates that particle size has a substantial effect on the magnetic properties of cemented carbide. Fine and ultrafine WC particles, due to their higher chemical reactivity and good sintering performance, can promote the diffusion and bonding of the Co binder, thus enhancing the stability of the material’s magnetic performance. However, smaller particle sizes may lead to increased porosity and inclusions, affecting the material’s hardness and magnetic performance. Therefore, the choice of particle size should be tailored to the specific application needs when preparing cemented carbide.

Regarding the atmosphere, cemented carbide bars sintered under vacuum and argon atmospheres exhibited higher coercive force and better magnetic stability. This is because these atmospheres effectively control the oxygen content and volatile elements, reducing porosity and inclusions, and promoting clearer grain boundaries and grain growth. In contrast, cemented carbide bars sintered in a hydrogen atmosphere showed significantly lower magnetic saturation. This is likely due to the decarburizing effect of hydrogen. Therefore, selecting the appropriate sintering atmosphere is crucial for obtaining cemented carbide bars with excellent magnetic properties. Further improvements in cemented carbide performance can be achieved by optimizing sintering process parameters and adding suppressants.

September 4, 2024

Meilleur matériaux TOP

Schreibe einen Kommentar

Deine E-Mail-Adresse wird nicht ver?ffentlicht. Erforderliche Felder sind mit * markiert.

二次元男生操女生屁眼爽| 大肌巴日小个子女人视频| 任你橹在线久久精品9| 少妇被黑人到高潮喷出白浆| 91精品国产剧情欧美一区二区| 色偷偷影音先锋男人av| 欧美 亚洲 日本 国产| 欧美人与兽大屌肛交爆菊| 99久久99久久精品视频| 在线精品亚洲观看不卡欧| 新视觉亚洲三区二区一区理伦| 男的鸡巴插女的视频| 无码一区二区三区色哟哟| 99久久精品国产一区二区成人了| 日本黑鸡吧黄色录像| 亚洲激情无码视频| 日本精品高清在线观看| 男人的下面进女人的下面在线观看| 日本亚洲欧洲一区二区| 精品久久久久中文字幕人| 精品一区二区av天堂色偷偷| 欧美性做爰片免费视频看| 中文字幕人妻一区二区三区久久| 欧美一区亚洲一区视频在线观看| 久久高清中文字幕第一页| 欧美一级淫片免费播放口| 性一交一子一伦一乱| 日韩精品一区二区天堂| 欧美日韩视频在线一区二区| 美女被插b在线观看| 欧美性爱撅臀插入啪啪啪| 男人的天堂日本在线观看| 中文字幕国产精品一区二区三区| 日韩激情精品久久久一区二区| 欧美成人精品一区二区免费看| 看女生b免费视频| 中国熟女色av夜夜嗨| 精品无码国产一区二区三区A| 国产青青操骚货在线观看| 69国产成人综合久久精| 2021最新热播国产一区二区|